How to repair and utilize drilling mud pump crankshaft effectively
Drilling mud pump, commonly known as the heart of a drilling rig, is one of the most important equipment of oil rig. It needs to transport the liquid with high viscosity, high density, high grindability, and strong corrosiveness under high pressure, working in harsh environments and with high alternating loads. It is often found that the journal surface of the crankshaft bearing is seriously worn during repair, which is also the most common failure of the crankshaft. However, the crankshaft is the most expensive part of the pump, so it is very important to repair and use it. The traditional repair methods such as EFI plating and bushing method are cumbersome and cannot achieve ideal results. For those with less serious wear, Loctite adhesive is used, which is convenient, fast, economical, energy-saving, and also increases the connection strength; for those with serious wear, it can be repaired by welding, which can achieve the original performance.
Wear of crankshaft in drilling mud pump
Due to reasons such as assembly or too much impact, after a period of on-site use of drilling mud pumps, it is often found that the main bearing of the crankshaft runs into the inner circle. After the drilling pump disintegrates, careful inspection will find that the journal and the main bearing inner rail move and rub against each other, resulting in wear and tear. The bearing pressure plate and the side of the inner track of the bearing are shiny, and the gap is measured with a feeler gauge, and serious bearings will fall off. According to assembly standards, all main bearings and crankshaft journals have interference fit, which may result in clearance fit or failure to meet fit requirements after wear, reducing connection strength and requiring timely handling.Compare the data of the worn area measured with an external micrometer with the original size, according to years of on-site repair experience, it is concluded that Loctite adhesive is used for treatment when the gap is less than 0.254mm, and when the gap exceeds 0.254mm, repair the welding and then on the lathe to reach the required size.
The bonding method of Loctite adhesive
The Loctite 600 series adhesive is an anaerobic cylindrical holding adhesive with strong holding performance, suitable for the bearings, gears, pulleys, and shafts.The use of Loctite bonding technology can replace EFI plating and replace the interference fit with facing-up. It can also greatly increase the strength of the interference fit, which generally increases the shear strength by more than 2 times.
When the gap is less than 0.127mm, the Loctite 609 is used, and when the gap is less than 0.254mm, the Loctite 680 is used. Although the maximum gap that 660 can repair is 0.54mm, if the gap is too large, the concentricity error between the crankshaft and bearings will be too large, so it is not recommended to use it.
The specific implementation process of using Loctite adhesive: The first is to clean the bonding surface. Remove the burrs on the mating surface of the crankshaft journal, clean all bonding surfaces with dilute hydrochloric acid to remove rust, rinse the residues with water, and then use 755 Loctite cleaning agent for final cleaning. The second is to apply glue. Apply 609 or 680 Loctite evenly to the crankshaft journal mating surface and spray 7649 or 7471. The third is to install bearings. Heat the main bearing with an oil bath to a temperature of 90-100 ℃, clean the inner rail of the bearing, and install it directly in place. The fixed curing time is 10 minutes, the full curing time is 24 hours, and the working temperature is -54~149 ℃.
Welding repair method
When the gap is less than 0.254mm, the surfacing welding process can meet the use requirements. The submerged-arc-welding device has a high welding current and large deformation of the welded parts, which cannot meet the repair of the crankshaft. Manual metal-arc welding and carbon dioxide arc welding have moderate costs, low welding currents, small deformation of the welded parts, and will not change the structure and performance of the original materials. The material of the drilling pump crankshaft is 35CrMo medium carbon tempered steel.
Choose welding wire with a composition similar to that of 35CrMo medium carbon tempered steel to meet the principle of equal welding quality. 35CrMo is an alloy structural steel with poor weldability and large crack tendency, so it is necessary to strictly control the welding process conditions for pre-welding and post-welding heat treatment. The poor welding performance of 35CrMo is mainly manifested in two aspects: firstly, the embrittlement and softening of the welding heat affected zone.Due to the high carbon content and numerous alloying elements in medium carbon tempered steel, the steel has a strong tendency to harden, resulting in the production of a large amount of martensite in the quenching zone of the heat affected zone, leading to severe embrittlement. When the heat-affected zone is heated to an area that exceeds the tempering temperature during the tempering treatment, a softening zone with a strength and hardness lower than that of the base material will appear. Second, the crack tendency is serious. The hardening tendency of the medium carbon tempered steel is large, and the martensitic structure generated in the heat affected zone increases the cold cracking tendency of the welded joint. In addition, the medium carbon tempered steel has high content of carbon and alloying elements, a wide range of crystallization temperatures in the melt pool, severe segregation, so it has a greater sensitivity to thermal cracks.
Preheat to 150-200 ℃ before welding, and ensure that the crankshaft welding temperature is not lower than 150 ℃ during the welding process. Oxygen acetylene flame or other heating methods can be used to ensure its temperature. When welding, the welding speed should be adjusted according to the degree of wear, and the welding coating should be cleaned in time to prevent the occurrence of welding slag. After welding, wrap in felt and cool to room temperature. If the weather is too cold, put in a heated house.In order to prevent thermal cracks, it is required that the welding wire used is low-carbon welding wire, and the carbon mass fraction in the welding wire should be controlled within 0.15, with a maximum of 0.25, and the mass fractions of sulfur and phosphorus should be less than O.03-0.035.
After the crankshaft is cooled, the upper lathe starts to turn, and the finishing turning is carried out when the size is reached to ensure required roughness before removal. The main bearing is installed into the bearing sleeve, and heat it in an oil bath to 80-100 ℃, and the crankshaft can be assembled, and the assembly is in place. When the natural temperature is too cold, the crankshaft journal should be preheated to around 40 ℃ before assembly to prevent the bearing inner rail from cracking due to a large temperature difference in heat transfer. Tempering will occur when the bearing is heated to more than 120℃ in the oil bath, so it is necessary to control the temperature.
Good field application of technology
According to the degree of wear, Loctite adhesive bonding process or welding repair process is reasonably selected. The service performance of repaired crankshaft is close to that of the original. Tracking the usage, the drilling team reported that the use effect is good and can meet the requirements.
On the basis of satisfying the repair, the application of this method can greatly save the material cost, and the repair process is simple and strong operability. The repair process can also be applied to repair other worn shafts.